Eight common welding defects from a visual inspector's view: which you can see on the surface, which stay hidden, their causes and which NDT method finds them.

By Syed Hasan25 Nov 20269 min read

Welding Defects You Can See, and the Ones You Cannot

A weld can look smooth, even and tidy and still be unfit for service. It can also look rough and turn out to be perfectly sound. That is the uncomfortable truth every visual welding inspector learns early: the surface tells you a lot, but not everything, and the skill is knowing which welding defects your eyes can actually find and which ones need another method.

This post takes eight common welding defects and sorts them the way a visual inspector does at the joint: those you can see on the weld surface, those you can only see from the root side, and those that are hidden inside. For each one you get what to look for, the usual cause and how to prevent it, plus which NDT method picks up what visual inspection misses.

Imperfection or defect: get the word right first

Not every irregularity in a weld is a defect. ISO 6520-1 classifies the geometric imperfections a weld can contain. Whether an imperfection becomes a defect depends on the acceptance criteria that apply: an imperfection is any departure from the ideal weld, and a defect is an imperfection that exceeds the acceptance limits for that job.

Those limits come from the governing code or standard and the project specification. ISO 5817 sets quality levels for fusion-welded joints in steel and some other metals, labelled B, C and D, with B the most demanding. Structural work may follow AWS D1.1, process piping ASME B31.3 and pipelines API 1104, and each sets its own limits. So the inspector's report should name the imperfection, its size and location, and only then say whether it is acceptable under the stated criteria. "Undercut, 40 mm long at the cap toe" is a finding. "Bad weld" is not.

What visual inspection can and cannot do

For weld defects, visual inspection is the first and cheapest NDT method, and it is done at every stage, not only at the end. Before welding you check joint preparation, fit-up, cleanliness and the consumables. During welding you watch interpass cleaning and the root. After welding you check the profile, the size and the surface.

It only works under the right conditions. The surface has to be clean of slag and spatter, the light has to be good enough and come from the right angle, and you have to be able to get your eyes, or a mirror or borescope, close to the area. A magnifier helps with fine features. Many specifications and inspection procedures set minimum requirements for lighting and viewing; follow the ones that apply to your job, and record when access or lighting limited what you could see.

What visual inspection cannot do is see through metal. Anything below the surface, or on a root face you have no access to, needs another method. The rest of this post is built around that line.

Cross-section of a butt weld with surface imperfections marked in one colour and hidden imperfections inside the weld marked in another
What the eye can reach, and what stays buried inside the weld.

Welding defects you can see on the weld surface

1. Undercut

Undercut is a groove melted into the base metal at the weld toe and left unfilled. Look along both toes with a torch held low to throw a shadow, and measure the depth with a weld gauge. The usual causes are too much current, too fast a travel speed or the wrong electrode angle. Prevention is correct parameters and technique from the qualified procedure.

2. Overlap

Overlap is weld metal that has flowed beyond the toe and lies on the base metal without fusing to it. It looks like a rolled lip at the edge of the weld. It is easy to mistake for a generous profile, but the unfused edge acts like a notch. Causes include too low a travel speed, low current or a poor angle, often in fillet welds made in the horizontal position.

3. Spatter

Spatter is droplets of molten metal thrown out of the arc and stuck to the surface around the weld. In many specifications it is treated as a surface irregularity rather than a reason to reject on its own, but it still needs attention: it can hide other imperfections, interfere with coating and get in the way of surface NDT. Excess current, a long arc and contaminated consumables are the usual causes.

4. Surface porosity

Porosity is gas trapped in the weld metal as cavities. When the pores break the surface you can see them as small holes or a line of pinholes. Surface porosity is a warning sign, because where some gas reached the surface, more may be trapped below. Causes are moisture, oil or rust on the joint, damp consumables and poor gas shielding, for example from a draught on site.

5. Surface cracks

A crack is a fracture in the weld metal or the heat-affected zone. Some, such as cracks at the end of a weld crater or along a toe, can be seen with good lighting and magnification. Many are too fine to see by eye, which is why visual inspection alone should never be relied on to clear a weld of cracking. Cracks are normally treated as unacceptable under most codes.

Two cross-sections of a fillet weld toe, one with a groove melted into the base metal and one with weld metal rolled over the base metal unfused
Undercut cuts into the base metal; overlap rolls over it without fusing.

Defects you can see only from the root side

6. Incomplete penetration

Incomplete penetration means the weld metal has not reached through the required joint thickness at the root. On a plate or a large pipe with root access, it shows up as an unfused root edge or a gap along the root. On a small-bore pipe with no access, it is invisible from outside. Causes are too small a root gap, too large a root face, low current or fast travel. Good fit-up is the main prevention, which is why the inspector checks it before the first run is laid.

Defects visual inspection cannot find

7. Slag inclusion

Slag inclusion is nonmetallic slag trapped inside the weld metal, usually between runs. It forms when slag from one run is not fully removed before the next. You will not see it on the finished weld; you might see the conditions that cause it during welding, such as poor interpass cleaning or a deep notch between runs. Thorough cleaning between passes prevents it.

8. Lack of fusion

Lack of fusion is where the weld metal fails to fuse with the base metal or with a previous pass. At the toe it can sometimes be seen; on the sidewall of the groove or between runs it is buried. It is one of the more dangerous imperfections because it is flat, like a crack. Causes are low heat input, wrong electrode angle and dirty or badly prepared surfaces.

Buried porosity and subsurface cracks belong in this group too.

Which NDT method finds what visual inspection misses

MethodFinds bestLimitation
Visual (VT)Profile, undercut, overlap, spatter, surface poresSurface only, and only what you can reach and light
Penetrant (PT)Fine surface-breaking cracks and poresOnly flaws open to the surface
Magnetic particle (MT)Surface and near-surface cracksFerromagnetic materials only
Ultrasonic (UT)Planar flaws: lack of fusion, cracksNeeds skilled operators and suitable geometry
Radiography (RT)Volumetric flaws: porosity, slag, incomplete penetrationCan miss planar flaws not aligned with the beam

The method and the extent of testing are set by the code and the project specification, not chosen on the day. How these imperfections appear on film is covered in reading weld radiographs, which picks up where this post stops.

Photograph of an inspector's gloved hands holding a weld gauge and a torch against a fillet weld on a steel plate
A low torch angle and a weld gauge find most surface imperfections.

Eight is not the whole list

The eight above are the ones most often taught together, but a real inspection checklist is longer. Burn-through, excess weld metal or reinforcement, root concavity, arc strikes on the parent metal, misalignment between members and crater cracks all appear in the standards and on real jobs. An arc strike in particular is easy to ignore and can start a crack in hardenable steels.

The prevention list behind almost all of them is the same: the right process and parameters from a qualified procedure, proper joint preparation and fit-up, clean base metal, suitable filler with correct storage and handling, sound technique and interpass cleaning, and visual inspection backed by suitable NDT at the right stage.

Frequently asked questions

What are the most common welding defects?

The eight most often taught together are undercut, overlap, spatter, porosity, cracks, incomplete penetration, slag inclusion and lack of fusion. A real inspection checklist is longer, adding burn-through, excess weld metal, root concavity, arc strikes, misalignment and crater cracks. Whether any of them is rejectable depends on the acceptance criteria for the job.

What is the difference between a weld imperfection and a weld defect?

An imperfection is any departure from the ideal weld; ISO 6520-1 classifies them. It becomes a defect only when it exceeds the acceptance limits that apply, set by the governing code, such as ISO 5817, AWS D1.1, ASME B31.3 or API 1104, and the project specification. So report the imperfection and its size first, then judge it.

Can visual inspection find all weld defects?

No. It finds what is on a surface you can clean, light and reach: undercut, overlap, spatter, surface pores and some cracks. Slag inclusion, buried porosity, lack of fusion on the sidewall and subsurface cracks are inside the weld, so ultrasonic testing or radiography is needed, with penetrant or magnetic particle testing for fine surface cracks.

What causes porosity in welding?

Gas trapped in the weld metal as it solidifies. The usual sources are moisture, oil or rust on the joint, damp consumables and poor gas shielding, for example from a draught on site. Pores that break the surface are a warning sign, because where some gas reached the surface, more may be trapped below it.

Where to go next

Finding, measuring and reporting surface imperfections is the core of the CSWIP 3.0 visual welding inspector preparation, and the CSWIP 3.1 welding inspector preparation takes it into procedures and NDT. If you are comparing routes, API 577 vs CSWIP 3.1 and CSWIP 3.1 vs AWS CWI set them side by side, and the welding repair and inspection course covers what happens after a defect is found.

Related reading: How to Read Welding Symbols on Engineering Drawings, WPS and PQR Review: A Welding Inspector's Checklist.

Exam preparation

Preparing for CSWIP 3.0?

Practise with exam-style questions, timed mocks and study notes. 400 questions in the bank.

Also relevant: CSWIP 3.1 Welding Inspector, API 577 Welding Inspection and Metallurgy

  • Welding
  • Weld defects
  • Visual inspection
  • NDT
  • CSWIP 3.0
  • +1
Share

Related Certifications

Certifications covered in this article. Each guide has the exam format, eligibility route and a practice question bank.