Pitting corrosion is the damage that makes a thickness survey lie. You take a grid of readings, every one of them close to the original wall, and a month later the line is weeping through a hole you could cover with a pencil tip. The metal around the hole looks almost new. The problem was never how much metal was lost; it was where.
This post covers pitting corrosion in depth: what starts a pit, why it keeps growing once it has started, where it turns up in plant, which inspection methods actually find it, and how engineers decide whether pitted equipment can stay in service. It goes further than the short pitting entry in a general list of corrosion types, and it should leave you able to plan an inspection for a pitting threat rather than hope a thickness grid catches it.
How a pit starts
Most pitting starts where a protective surface film breaks down at a few small spots. Stainless steels, aluminium and many other alloys rely on a thin passive oxide film for their corrosion resistance. Chloride ions are the classic film breaker: they attack weak points in the film and stop it from repairing itself.
Weak points are not hard to find. Common initiation sites include:
- non-metallic inclusions at the surface, such as manganese sulfides in some stainless grades;
- scratches, weld spatter, embedded iron from carbon steel tools and other surface damage;
- crevices and the edges of deposits, where chemistry inside differs from the bulk fluid;
- heat tint and weld discolouration that has not been removed after fabrication.
Plenty of pits start and then heal again when the film repairs. The ones that matter are those that survive long enough to set up their own local chemistry, and from that point they tend to keep going.
Why pits keep growing
A pit that survives becomes a small, self-sustaining corrosion cell. Inside it, a tiny area of exposed metal acts as the anode. The large area of passive surface around it acts as the cathode, taking up the oxygen reduction reaction. A small anode driven by a large cathode corrodes fast.
The chemistry inside the pit then makes matters worse. Metal ions dissolving in the pit react with water and release acid, and chloride ions migrate in to balance the charge. The pit fills with an increasingly acidic, chloride-rich solution in which the passive film cannot reform. This is why pitting is called autocatalytic: the pit makes the conditions that keep it growing, and it grows down into the wall faster than it grows across the surface.
Pits also come in different shapes, and the shape changes how dangerous a pit is. Some are narrow and deep, some wide and shallow, and some undercut, opening into a larger cavity below a small mouth. An undercut pit can hide a large amount of metal loss behind a surface opening that looks trivial.
Where pitting corrosion turns up in plant
Pitting is a threat to carbon steel as well as to passive alloys, but the conditions differ. This table is the first-guess list most inspectors carry in their heads.
| Location | Material | Usual driver |
|---|---|---|
| Seawater and cooling-water service | Austenitic stainless steel | Chlorides, warm water, low flow |
| Under insulation | Stainless and carbon steel | Wet insulation leaching chlorides |
| Line bottoms and low points | Carbon steel | Water and solids settling, under-deposit attack |
| Dead legs and idle equipment | Any | Stagnant water, microbial activity |
| Tank floors | Carbon steel | Water and sludge on the product side, soil on the underside |
| Boiler and feedwater systems | Carbon steel | Dissolved oxygen |
Stagnation is the common thread. Flowing, clean fluid tends to keep surfaces uniform; still water lets deposits, oxygen differences and microbes concentrate the attack. Microbiologically influenced corrosion often shows up as clusters of pits, which is covered in the MIC guide. Where chlorides and tensile stress act together on austenitic stainless steel, pits can also become the starting point for cracking, explained in chloride stress corrosion cracking of stainless steel.
How to find pitting
The basic difficulty is scale. A pit can be a few millimetres across, and a spot ultrasonic reading samples a small patch under the probe. Unless the probe happens to sit on the pit, the reading shows full wall. Finding pitting therefore means scanning, not sampling.
- Visual inspection after cleaning during internal entry. Pits hide under scale and deposits, so cleaning comes first.
- Pit depth gauge for accessible surfaces, measuring each significant pit directly.
- Replica or moulding compound pressed into a pitted area, then measured away from the equipment, useful where a gauge cannot reach the bottom of a pit.
- Ultrasonic scanning: continuous scanning or automated and phased array mapping over an area, rather than a few spot readings, to find the minimum wall.
- Magnetic flux leakage for tank floors and for pipelines through in-line inspection tools, covering large areas quickly before follow-up with UT.
- Profile radiography on small-bore piping, where pits show as local loss on the wall profile.
- 3D laser scanning for external pitting, giving a depth map that can be used directly in an assessment.
Corrosion coupons in the process stream also tell you about pitting, not just a general rate, if someone examines and measures the pits on them. The difference between coupons, ER and LPR probes is set out in corrosion coupons vs ER probes vs LPR.
How to assess pitted equipment
Once you have the data, assessment answers one question: is there enough wall left, now and at the next inspection? A useful order of work:
- Characterise the pitting. Record the deepest pits, the density (how many per area), the size of the pitted region and whether pits are isolated, clustered or lined up.
- Compare the deepest pit with the required thickness. The remaining wall under the deepest pit is the starting point, but widely scattered pits are often assessed differently from a general corroded area.
- Work out a pitting rate. Repeat measurements on the same pits give a growth rate. Pit growth is often not steady, so treat a single interval with caution.
- Use the code that applies. API 579-1/ASME FFS-1 has a dedicated part for pitting, using pit-couple measurements and standard pit charts to judge the effect on strength. Tank shells have their own rules in API 653, discussed in API 653 corroded areas and pitting on tank shells.
- Set the next inspection and the repair or mitigation. A pass today is only useful with a date attached.
Engineers sometimes describe pitting with a pitting factor: the depth of the deepest pit divided by the average metal penetration. A factor near one means the attack is close to uniform; a large factor tells you an average-loss calculation will badly understate the risk.
How to prevent pitting corrosion
Prevention follows from the mechanism.
- Choose the right alloy for the chloride level and temperature. Molybdenum-bearing stainless grades and duplex grades resist pitting better than basic austenitic grades, and the pitting resistance equivalent number, worked out from chromium, molybdenum and nitrogen content, is the usual way to rank them.
- Keep surfaces clean. Remove deposits, keep flow above the point where solids settle, and drain idle equipment rather than leaving it full of still water.
- Finish fabrication properly. Remove heat tint, embedded iron and spatter from stainless steel, and pickle and passivate where the specification requires.
- Control the water. Oxygen removal in boiler systems, chloride control, biocides and corrosion inhibitors where the process allows.
- Use coatings and cathodic protection on carbon steel where the service suits them, such as tank floors.
Frequently asked questions
What causes pitting corrosion?
Pitting starts where a protective surface film breaks down at a few small spots, most often because of chlorides, and at weak points such as inclusions, scratches, deposits and heat tint. A pit that survives becomes a small anode driven by a large cathode, and the acidic, chloride-rich solution inside it stops the film from reforming.
How do you measure pit depth?
On accessible surfaces, clean the area and use a pit depth gauge on each significant pit, or press a replica compound into the pits and measure it later. For larger areas, ultrasonic scanning or phased array mapping finds the minimum wall, magnetic flux leakage screens tank floors and pipelines, and 3D laser scanning maps external pits.
Why does UT thickness testing miss pits?
A spot ultrasonic reading only samples the small patch under the probe. Pits can be a few millimetres across, so unless the probe sits on one, the reading shows full wall. Finding pitting means scanning continuously over an area, or mapping it with automated or phased array UT, rather than taking a few grid readings.
Which stainless steel resists pitting best?
Grades with more molybdenum, and duplex grades, resist pitting better than basic austenitic grades. Engineers rank alloys with the pitting resistance equivalent number, worked out from chromium, molybdenum and nitrogen content. The right choice still depends on the actual chloride level and temperature, and on keeping surfaces clean and free of deposits.
What to do next
When pitting is on your threat list, write it into the inspection plan by location and by method: name the low points, dead legs and stagnant zones, and specify scanning, not spot readings. Recognising pitting and the conditions behind it is a core part of the API 571 corrosion and materials certification preparation, and assessing pitted components is worked through in the API 579-1 fitness-for-service programme.
Exam preparation
Preparing for API 571?
Practise with exam-style questions, timed mocks and study notes. 3,357 questions in the bank.