Welcome to Excellence Integrity Management - Empowering Professionals Globally.

Heat Exchanger Corrosion: Where It Happens and How to Prevent It

Heat exchanger corrosion explained: tube side vs shell side, eight common mechanisms, how fouling feeds corrosion, and practical ways to prevent it.

By Siddique28 Nov 20269 min read

Heat Exchanger Corrosion: Where It Happens and How to Prevent It

A heat exchanger is about the worst place you could design for a piece of metal to live. Thin tubes, two different fluids, a temperature difference across every wall, crevices at every joint, and often cooling water that is warm, aerated and full of life. It is no surprise that heat exchanger tube corrosion, ending in a tube leak, is one of the most common reasons an exchanger comes out of service early.

This post looks at heat exchanger corrosion specifically: which side of the tube it attacks, the mechanisms that cause most failures, how fouling and corrosion make each other worse, and the practical steps that prevent it. Fouling itself and the parts of the exchanger are covered in their own posts, linked below, so this one stays on the metal loss and cracking.

Tube side or shell side: where the attack starts

The first question in any exchanger failure is which fluid did the damage. In a typical shell and tube cooler, cooling water runs through the tubes and the process fluid runs on the shell side, though designers sometimes swap them. Each side brings its own threats.

The water side usually carries the threats of oxygen, chlorides, deposits and bacteria. Water velocity varies from the inlet to the outlet, and wherever flow is low, solids settle and the surface underneath begins to corrode. The process side brings whatever the stream contains: acid gases, chlorides carried over from upstream, ammonia, or condensing water that is far more aggressive than the bulk fluid. If you need a refresher on which part is which, see inside a shell and tube heat exchanger.

Knowing the side narrows the list of suspects quickly. A pit that starts on the bore of a water-side tube and a crack that starts on the outside of the same tube have different causes and different fixes.

Cutaway diagram of a shell and tube heat exchanger showing cooling water in the tubes, process fluid on the shell side and the typical damage on each side
Which side did the damage start on? Water side and process side bring different threats.

The heat exchanger corrosion mechanisms behind most failures

The causes are rarely exotic. A handful of mechanisms account for most of what inspectors find at a turnaround.

1. Under-deposit corrosion

Scale, silt, corrosion products and biological slime settle on tube walls, especially in low-velocity zones. The pocket under the deposit loses contact with the bulk water and develops its own, more aggressive chemistry, so local pits grow beneath the deposit while the open surface nearby looks fine. This is the main reason fouling and corrosion travel together.

2. Pitting

Stainless steel and some other alloys depend on a thin protective film. Chlorides in cooling water or in the process can break that film down at small spots, and the attack then concentrates there. A few pits can perforate a thin tube wall while the rest of the tube is untouched, which is why pitting is so often the cause of a single leaking tube.

3. Galvanic corrosion at the tubesheet

When the tubes and the tubesheet or channel are made of different metals and the joint is wetted, the less noble metal corrodes faster. A copper alloy tube bundle in a carbon steel tubesheet is a familiar example, with the steel around the tube holes losing metal. Water boxes on seawater coolers are often fitted with sacrificial anodes for this reason.

4. Erosion-corrosion at the tube inlet

Water entering the tubes is turbulent for a short length before the flow settles. That turbulence strips the protective film and the metal under it, so the first part of each tube can thin far faster than the rest. The damage is concentrated near the tube ends on the inlet side, and it is worse when the water carries sand or silt.

5. Microbiologically influenced corrosion

Bacteria living in slime layers on cooling-water surfaces change the chemistry right at the metal and drive deep, local attack, often under nodules or tubercles. Stagnant periods, such as an exchanger left full of water during a shutdown, make it much worse. The mechanism is covered in detail in the MIC guide.

6. Stress corrosion cracking

Where the material is susceptible, the right combination of tensile stress and environment cracks the metal with little visible metal loss. Austenitic stainless steels can crack in hot chloride environments, and copper alloys such as brass can crack where ammonia is present. Residual stress from tube rolling at the tubesheet adds to the risk at the tube ends.

7. Crevice corrosion

Tight gaps, such as where a tube passes through a baffle or sits in the tubesheet hole behind the rolled joint, hold stagnant fluid. The chemistry inside the crevice changes and localised attack follows. It is easy to miss because the damage hides inside the joint.

8. Dealloying

Some alloys lose one element selectively. Dezincification of brass is the classic case: zinc is removed and leaves a weak, porous copper layer that keeps its shape but has lost its strength. The tube can look intact and still fail under pressure.

Close-up photograph of a tubesheet face with thinned and grooved tube ends at the inlet side of a cooling water exchanger
Inlet-end erosion-corrosion: the first length of each tube takes the turbulence.

How fouling and corrosion feed each other

Fouling and corrosion are usually discussed separately, but in an exchanger they form a loop. Deposits create the conditions for under-deposit corrosion and give bacteria a home. Corrosion products then add to the deposit, so the layer gets thicker, flow drops further and more solids settle. Reduced flow also raises the wall temperature on the hot side, which speeds up scaling.

Breaking the loop at either point helps the other. Keeping tubes clean slows corrosion, and controlling corrosion reduces the iron oxide that becomes part of the fouling. The causes and cleaning methods for deposits are covered in fouling in heat exchangers; the point here is that a cleaning programme is also a corrosion control measure.

Quick guide: mechanism, location, prevention

MechanismWhere it usually appearsMain prevention
Under-depositLow-velocity tubes, bottom of the bundleVelocity control, cleaning, water treatment
PittingStainless tubes with chloridesMaterial suited to the chloride level
GalvanicTubesheet and channel around tube holesCompatible metals, anodes, coatings
Inlet erosion-corrosionFirst length of the tubes, inlet endVelocity limits, inlet tube inserts
MICCooling-water side, stagnant periodsBiocide, flow, draining when idle
Stress corrosion crackingRolled tube ends, hot chloride or ammonia serviceMaterial choice, stress relief
CreviceBaffle holes, tube-to-tubesheet jointsJoint design, avoid stagnant gaps
DealloyingBrass tubes in aggressive waterInhibited alloys or a different alloy

What a failed tube tells you

A removed tube, split along its length, is the best evidence you will get. Each mechanism leaves a recognisable signature if you know what to look for.

Pits clustered under a layer of deposit on the bore point to under-deposit attack or MIC; if the deposit forms raised nodules with deep pits beneath, bacteria are the stronger suspect. Smooth, grooved thinning that is worst near one end and fades along the tube points to inlet erosion-corrosion. Fine branching cracks with almost no metal loss point to stress corrosion cracking. A copper-coloured, spongy layer on a brass tube that crumbles when scraped points to dezincification.

Record where the tube sat in the bundle as well. Damage concentrated in the bottom rows, the first pass or the tubes near the inlet nozzle says as much about the cause as the damage itself.

Photograph of a heat exchanger tube split lengthwise, showing pits under a layer of deposit on the inside surface
A split tube shows which side the damage started on and what drove it.

How to prevent corrosion in a heat exchanger

Preventing heat exchanger corrosion starts at design and continues every day the exchanger runs. The measures that matter most are these.

Choose the material for the real fluid. Base the tube material on the actual chloride level, temperature, oxygen and contaminants, including upsets, not on the design-case composition alone. Check that the tubes and tubesheet are compatible if both are wetted.

Treat the water. Cooling water corrosion, scale and biological growth need one programme that covers all three, with someone checking the results, not just the dosing pump.

Keep velocity in range. Too low and solids settle; too high and the tube inlets erode. Running an exchanger far below its design flow for long periods is a common, quiet cause of deposit-driven failures.

Clean on condition and protect during idle time. Clean when performance or inspection shows deposits building, not only on a calendar. Drain and dry, or circulate treated water, rather than leaving an exchanger standing full of water during a shutdown.

Frequently asked questions

What causes corrosion in heat exchangers?

Mostly a handful of mechanisms: under-deposit attack, chloride pitting of stainless tubes, galvanic corrosion at the tubesheet, erosion-corrosion at the tube inlet, microbiologically influenced corrosion, stress corrosion cracking, crevice attack and dealloying. Thin tubes, two fluids, crevices at every joint and warm, aerated cooling water give each of them easy conditions.

What causes tube inlet erosion in a heat exchanger?

Water entering the tubes is turbulent for a short length before the flow settles, and that turbulence strips the protective film and the metal under it. The first part of each tube on the inlet side can thin far faster than the rest, and sand or silt in the water makes it worse. Velocity limits and inlet tube inserts are the usual remedies.

Does fouling cause corrosion in a heat exchanger?

Yes, and the two feed each other. Deposits create the pocket chemistry for under-deposit corrosion and give bacteria a home, then corrosion products thicken the deposit and cut flow further. That is why a cleaning programme also counts as a corrosion control measure, and controlling corrosion reduces the iron oxide in the fouling.

How do you find out what caused a tube leak?

Pull a sample tube, split it along its length and read the signature. Pits under deposit suggest under-deposit attack or MIC, grooved thinning near one end suggests inlet erosion-corrosion, fine branching cracks suggest stress corrosion cracking, and a spongy copper layer on brass suggests dezincification. Record where the tube sat in the bundle too.

What to do next

When a tube leaks, resist the urge to plug it and move on. Pull a sample tube, split it, and look at which side the damage started on and what it looks like. That single step tells you which mechanism you are dealing with and which of the measures above will stop the next leak. For a structured approach to exchanger inspection and repair decisions, the heat exchanger inspection and maintenance course covers the practical side, and the heat exchanger integrity and tube bundle assessment programme goes into damage mechanisms and bundle life in depth.

Exam preparation

Preparing for API 571?

Practise with exam-style questions, timed mocks and study notes. 3,357 questions in the bank.

  • Heat exchangers
  • Corrosion
  • Damage mechanisms
  • Cooling water
  • Tube failures
  • +1
Share

Related Certifications

Certifications covered in this article. Each guide has the exam format, eligibility route and a practice question bank.